 Brinell Hardness  Vickers Hardness  Rockwell Hardness  Tensile Strength
 100 HB   105 HV   – HRC   335 N/mm2
 101 HB   106 HV   – HRC   338 N/mm2
 102 HB   107 HV   – HRC   341 N/mm2
 103 HB   108 HV   – HRC   344 N/mm2
 104 HB   109 HV   – HRC   347 N/mm2
 105 HB   110 HV   – HRC   350 N/mm2
 106 HB   111 HV   – HRC   355 N/mm2
 107 HB   112 HV   – HRC   360 N/mm2
 108 HB   113 HV   – HRC   365 N/mm2
 109 HB   114 HV   – HRC   370 N/mm2
 110 HB   115 HV   – HRC   373 N/mmø
 111 HB   116 HV   – HRC   376 N/mm2
 112 HB   117 HV   – HRC   379 N/mm2
 113 HB   118 HV   – HRC   382 N/mm2
 114 HB   119 HV   – HRC   385 N/mm2
 115 HB   120 HV   – HRC   388 N/mm2
 116 HB   121 HV   – HRC   391 N/mm2
 117 HB   122 HV   – HRC   394 N/mm2
 118 HB   123 HV   – HRC   397 N/mm2
 119 HB   125 HV   – HRC   400 N/mm2
 120 HB   126 HV   – HRC   403 N/mm2
 121 HB   127 HV   – HRC   406 N/mm2
 122 HB   128 HV   – HRC   409 N/mm2
 123 HB   129 HV   – HRC   412 N/mm2
 124 HB   130 HV   – HRC   415 N/mm2
 125 HB   131 HV   – HRC   418 N/mm2
 126 HB   132 HV   – HRC   422 N/mm2
 127 HB   133 HV   – HRC   426 N/mm2
 128 HB   135 HV   – HRC   430 N/mm2
 129 HB   136 HV   – HRC   434 N/mm2
 130 HB   137 HV   – HRC   438 N/mm2
 131 HB   138 HV   – HRC   442 N/mm2
 132 HB   139 HV   – HRC   446 N/mm2
 133 HB   140 HV   – HRC   450 N/mm2
 134 HB   141 HV   – HRC   453 N/mm2
 135 HB   142 HV   – HRC   456 N/mm2
 136 HB   143 HV   – HRC   459 N/mm2
 137 HB   144 HV   – HRC   462 N/mm2
 138 HB   145 HV   – HRC   465 N/mm2
 139 HB   146 HV   – HRC   468 N/mm2
 140 HB   147 HV   – HRC   471 N/mm2
 141 HB   148 HV   – HRC   474 N/mm2
 142 HB   149 HV   – HRC   477 N/mm2
 143 HB   150 HV   – HRC   480 N/mm2
 144 HB   151 HV   – HRC   484 N/mm2
 145 HB   152 HV   – HRC   488 N/mm2
 146 HB   153 HV   – HRC   492 N/mm2
 147 HB   155 HV   – HRC   495 N/mm2
 148 HB   156 HV   – HRC   498 N/mm2
 149 HB   157 HV   – HRC   501 N/mm2
 150 HB   158 HV   – HRC   504 N/mm2
 151 HB   159 HV   – HRC   507 N/mm2
 152 HB   160 HV   – HRC   510 N/mm2
 153 HB   161 HV   – HRC   515 N/mm2
 154 HB   162 HV   – HRC   520 N/mm2
 155 HB   163 HV   – HRC   525 N/mm2
 156 HB   164 HV   – HRC   530 N/mm2
 157 HB   165 HV   – HRC   532 N/mm2
 158 HB   166 HV   – HRC   534 N/mm2
 159 HB   167 HV   – HRC   537 N/mm2
 160 HB   168 HV   – HRC   539 N/mm2
 161 HB   116 HV   – HRC   542 N/mm2
 162 HB   170 HV   – HRC   545 N/mm2
 163 HB   171 HV   – HRC   549 N/mm2
 164 HB   172 HV   – HRC   553 N/mm2
 165 HB   173 HV   – HRC   557 N/mm2
 166 HB   174 HV   – HRC   560 N/mm2
 167 HB   175 HV   – HRC   563 N/mm2
 168 HB   176 HV   – HRC   566 N/mm2
 169 HB   177 HV   – HRC   569 N/mm2
 170 HB   179 HV   – HRC   572 N/mm2
 171 HB   180 HV   – HRC   575 N/mm2
 172 HB   181 HV   – HRC   579 N/mm2
 173 HB   182 HV   – HRC   583 N/mm2
 174 HB   183 HV   – HRC   587 N/mm2
 175 HB   184 HV   – HRC   591 N/mm2
 176 HB   185 HV   – HRC   595 N/mm2
 177 HB   186 HV   – HRC   598 N/mm2
 178 HB   187 HV   – HRC   601 N/mm2
 179 HB   188 HV   – HRC   604 N/mm2
 180 HB   189 HV   – HRC   607 N/mm2
 181 HB   190 HV   – HRC   610 N/mm2
 182 HB   191 HV   – HRC   613 N/mm2
 183 HB   192 HV   – HRC   617 N/mm2
 184 HB   193 HV   – HRC   621 N/mm2
 185 HB   194 HV   – HRC   625 N/mm2
 186 HB   195 HV   – HRC   628 N/mm2
 187 HB   196 HV   – HRC   631 N/mm2
 188 HB   197 HV   – HRC   634 N/mm2
 189 HB   199 HV   – HRC   637 N/mm2
 190 HB   200 HV   – HRC   640 N/mm2
 191 HB   201 HV   – HRC   644 N/mm2
 192 HB   202 HV   – HRC   648 N/mm2
 193 HB   203 HV   – HRC   652 N/mm2
 194 HB   204 HV   – HRC   656 N/mm2
 195 HB   205 HV   – HRC   660 N/mm2
 196 HB   206 HV   – HRC   663 N/mm2
 197 HB   207 HV   – HRC   667 N/mm2
 198 HB   208 HV   – HRC   671 N/mm2
 199 HB   209 HV   – HRC   675 N/mm2
 200 HB   210 HV   – HRC   678 N/mm2
 201 HB   211 HV   – HRC   681 N/mm2
 202 HB   212 HV   – HRC   684 N/mm2
 203 HB   213 HV   – HRC   687 N/mm2
 204 HB   214 HV   – HRC   690 N/mm2
 205 HB   215 HV   – HRC   693 N/mm2
 206 HB   216 HV   – HRC   696 N/mm2
 207 HB   217 HV   – HRC   699 N/mm2
 208 HB   218 HV   – HRC   702 N/mm2
 209 HB   220 HV   – HRC   705 N/mm2
 210 HB   221 HV   – HRC   708 N/mm2
 211 HB   222 HV   – HRC   711 N/mm2
 212 HB   223 HV   – HRC   714 N/mm2
 213 HB   224 HV   – HRC   717 N/mm2
 214 HB   225 HV   – HRC   720 N/mm2
 215 HB   226 HV   – HRC   724 N/mm2
 216 HB   227 HV   – HRC   728 N/mm2
 217 HB   228 HV   – HRC   732 N/mm2
 218 HB   229 HV   – HRC   736 N/mm2
 219 HB   230 HV   – HRC   740 N/mm2
 220 HB   231 HV   – HRC   744 N/mm2
 221 HB   232 HV   – HRC   748 N/mm2
 222 HB   233 HV   – HRC   752 N/mm2
 223 HB   234 HV   – HRC   755 N/mm2
 224 HB   235 HV   – HRC   758 N/mm2
 225 HB   236 HV   – HRC   761 N/mm2
 226 HB   237 HV   – HRC   763 N/mm2
 227 HB   238 HV   – HRC   767 N/mm2
 228 HB   240 HV   20.3 HRC   770 N/mm2
 229 HB   241 HV   20.5 HRC   773 N/mm2
 230 HB   242 HV   20.7 HRC   776 N/mm2
 231 HB   243 HV   20.9 HRC   779 N/mm2
 232 HB   244 HV   21.1 HRC   782 N/mm2
 233 HB   245 HV   21.3 HRC   785 N/mm2
 234 HB   246 HV   21.5 HRC   788 N/mm2
 235 HB   247 HV   21.7 HRC   791 N/mm2
 236 HB   248 HV   21.9 HRC   793 N/mm2
 237 HB   249 HV   22.0 HRC   797 N/mm2
 238 HB   250 HV   22.2 HRC   800 N/mm2
 239 HB   251 HV   22.5 HRC   805 N/mm2
 240 HB   252 HV   22.7 HRC   810 N/mm2
 241 HB   253 HV   22.9 HRC   815 N/mm2
 242 HB   254 HV   23.1 HRC   820 N/mm2
 243 HB   255 HV   23.3 HRC   821 N/mm2
 244 HB   256 HV   23.5 HRC   824 N/mm2
 245 HB   257 HV   23.7 HRC   827 N/mm2
 246 HB   258 HV   23.9 HRC   831 N/mm2
 246 HB   258 HV   23.9 HRC   831 N/mm2
 247 HB   260 HV   24.0 HRC   835 N/mm2
 248 HB   261 HV   24.2 HRC   838 N/mm2
 249 HB   262 HV   24.3 HRC   841 N/mm2
 250 HB   263 HV   24.5 HRC   844 N/mm2
 251 HB   264 HV   24.7 HRC   847 N/mm2
 252 HB   265 HV   24.8 HRC   850 N/mm2
 253 HB   266 HV   25.0 HRC   853 N/mm2
 254 HB   267 HV   25.1 HRC   856 N/mm2
 255 HB   268 HV   25.3 HRC   859 N/mm2
 256 HB   269 HV   25.5 HRC   862 N/mm2
 257 HB   270 HV   25.6 HRC   865 N/mm2
 258 HB   271 HV   25.8 HRC   869 N/mm2
 259 HB   272 HV   26.0 HRC   873 N/mm2
 260 HB   273 HV   26.2 HRC   877 N/mm2
 261 HB   274 HV   26.4 HRC   880 N/mm2
 262 HB   275 HV   26.6 HRC   884 N/mm2
 263 HB   276 HV   26.7 HRC   888 N/mm2
 264 HB   277 HV   26.8 HRC   892 N/mm2
 265 HB   278 HV   26.9 HRC   896 N/mm2
 266 HB   280 HV   27.1 HRC   900 N/mm2
 267 HB   281 HV   27.3 HRC   903 N/mm2
 268 HB   282 HV   27.4 HRC   906 N/mm2
 269 HB   283 HV   27.5 HRC   909 N/mm2
 270 HB   284 HV   27.6 HRC   912 N/mm2
 271 HB   285 HV   27.8 HRC   915 N/mm2
 272 HB   286 HV   28.0 HRC   918 N/mm2
 273 HB   287 HV   28.1 HRC   921 N/mm2
 274 HB   288 HV   28.3 HRC   924 N/mm2
 275 HB   289 HV   28.4 HRC   927 N/mm2
 276 HB   290 HV   28.5 HRC   930 N/mm2
 277 HB   291 HV   28.7 HRC   935 N/mm2
 278 HB   292 HV   28.9 HRC   940 N/mm2
 279 HB   293 HV   29.0 HRC   945 N/mm2
 280 HB   294 HV   29.2 HRC   950 N/mm2
 281 HB   295 HV   29.3 HRC   953 N/mm2
 282 HB   296 HV   29.4 HRC   956 N/mm2
 283 HB   297 HV   29.5 HRC   959 N/mm2
 284 HB   298 HV   29.6 HRC   962 N/mm2
 285 HB   300 HV   29.8 HRC   965 N/mm2
 286 HB   301 HV   30.0 HRC   968 N/mm2
 287 HB   302 HV   30.2 HRC   971 N/mm2
 288 HB   303 HV   30.3 HRC   974 N/mm2
 289 HB   304 HV   30.4 HRC   977 N/mm2
 290 HB   305 HV   30.5 HRC   980 N/mm2
 291 HB   306 HV   30.6 HRC   983 N/mm2
 292 HB   307 HV   30.7 HRC   986 N/mm2
 293 HB   308 HV   30.8 HRC   989 N/mm2
 294 HB   309 HV   30.9 HRC   992 N/mm2
 295 HB   310 HV   31.0 HRC   995 N/mm2
 296 HB   311 HV   31.1 HRC   999 N/mm2
 297 HB   312 HV   31.2 HRC   1004 N/mm2
 298 HB   313 HV   31.3 HRC   1008 N/mm2
 299 HB   314 HV   31.4 HRC   1012 N/mm2
 300 HB   315 HV   31.6 HRC   1015 N/mm2
 301 HB   316 HV   31.8 HRC   1019 N/mm2
 302 HB   317 HV   31.9 HRC   1013 N/mm2
 303 HB   318 HV   32.0 HRC   1027 N/mm2
 304 HB   320 HV   32.2 HRC   1030 N/mm2
 305 HB   321 HV   32.3 HRC   1033 N/mm2
 306 HB   322 HV   32.4 HRC   1036 N/mm2
 307 HB   323 HV   32.5 HRC   1039 N/mm2
 308 HB   324 HV   32.6 HRC   1042 N/mm2
 309 HB   325 HV   32.7 HRC   1045 N/mm2
 310 HB   326 HV   32.8 HRC   1048 N/mm2
 311 HB   327 HV   32.9 HRC   1051 N/mm2
 312 HB   328 HV   33.0 HRC   1054 N/mm2
 312 HB   328 HV   33.0 HRC   1054 N/mm2
 313 HB   329 HV   33.1 HRC   1057 N/mm2
 314 HB   330 HV   33.3 HRC   1060 N/mm2
 315 HB   331 HV   33.4 HRC   1063 N/mm2
 316 HB   332 HV   33.6 HRC   1067 N/mm2
 317 HB   333 HV   33.7 HRC   1071 N/mm2
 318 HB   334 HV   33.8 HRC   1075 N/mm2
 319 HB   335 HV   33.9 HRC   1079 N/mm2
 320 HB   336 HV   34.0 HRC   1083 N/mm2
 321 HB   337 HV   34.1 HRC   1087 N/mm2
 322 HB   338 HV   34.2 HRC   1091 N/mm2
 323 HB   339 HV   34.4 HRC   1095 N/mm2
 324 HB   340 HV   34.5 HRC   1098 N/mm2
 325 HB   341 HV   34.6 HRC   1101 N/mm2
 326 HB   342 HV   34.7 HRC   1104 N/mm2
 327 HB   343 HV   34.9 HRC   1107 N/mm2
 328 HB   344 HV   35.0 HRC   1110 N/mm2
 329 HB   345 HV   35.1 HRC   1113 N/mm2
 330 HB   346 HV   35.2 HRC   1116 N/mm2
 331 HB   347 HV   35.3 HRC   1119 N/mm2
 332 HB   348 HV   35.4 HRC   1122 N/mm2
 333 HB   350 HV   35.5 HRC   1125 N/mm2
 334 HB   351 HV   35.6 HRC   1128 N/mm2
 335 HB   352 HV   35.7 HRC   1131 N/mm2
 336 HB   353 HV   35.9 HRC   1135 N/mm2
 337 HB   354 HV   36.0 HRC   1138 N/mm2
 338 HB   355 HV   36.1 HRC   1141 N/mm2
 339 HB   356 HV   36.2 HRC   1145 N/mm2
 340 HB   357 HV   36.3 HRC   1149 N/mm2
 341 HB   358 HV   36.4 HRC   1152 N/mm2
 342 HB   359 HV   36.6 HRC   1155 N/mm2
 343 HB   360 HV   36.7 HRC   1158 N/mm2
 344 HB   361 HV   36.9 HRC   1162 N/mm2
 345 HB   362 HV   37.0 HRC   1165 N/mm2
 346 HB   363 HV   37.1 HRC   1169 N/mm2
 347 HB   364 HV   37.2 HRC   1172 N/mm2
 348 HB   365 HV   37.3 HRC   1176 N/mm2
 349 HB   366 HV   37.4 HRC   1179 N/mm2
 350 HB   367 HV   37.5 HRC   1183 N/mm2
 351 HB   368 HV   37.6 HRC   1187 N/mm2
 352 HB   370 HV   37.7 HRC   1190 N/mm2
 353 HB   371 HV   37.8 HRC   1194 N/mm2
 354 HB   372 HV   38.0 HRC   1197 N/mm2
 355 HB   373 HV   38.1 HRC   1201 N/mm2
 356 HB   374 HV   38.2 HRC   1205 N/mm2
 357 HB   375 HV   38.4 HRC   1208 N/mm2
 358 HB   376 HV   38.5 HRC   1211 N/mm2
 359 HB   377 HV   38.6 HRC   1214 N/mm2
 360 HB   378 HV   38.7 HRC   1217 N/mm2
 361 HB   380 HV   38.8 HRC   1220 N/mm2
 362 HB   381 HV   38.9 HRC   1224 N/mm2
 363 HB   382 HV   39.0 HRC   1227 N/mm2
 364 HB   383 HV   39.1 HRC   1231 N/mm2
 365 HB   384 HV   39.2 HRC   1234 N/mm2
 366 HB   385 HV   39.3 HRC   1237 N/mm2
 367 HB   386 HV   39.4 HRC   1241 N/mm2
 368 HB   387 HV   39.5 HRC   1244 N/mm2
 369 HB   388 HV   39.6 HRC   1247 N/mm2
 370 HB   389 HV   39.7 HRC   1251 N/mm2
 370 HB   389 HV   39.7 HRC   1251 N/mm2
 371 HB   390 HV   39.8 HRC   1255 N/mm2
 372 HB   391 HV   39.9 HRC   1259 N/mm2
 373 HB   392 HV   40.0 HRC   1263 N/mm2
 374 HB   393 HV   40.1 HRC   1267 N/mm2
 375 HB   394 HV   40.2 HRC   1271 N/mm2
 376 HB   395 HV   40.3 HRC   1275 N/mm2
 377 HB   396 HV   40.4 HRC   1278 N/mm2
 378 HB   397 HV   40.5 HRC   1282 N/mm2
 379 HB   398 HV   40.6 HRC   1286 N/mm2
 380 HB   400 HV   40.8 HRC   1290 N/mm2
 381 HB   401 HV   40.9 HRC   1293 N/mm2
 382 HB   402 HV   41.0 HRC   1296 N/mm2
 383 HB   403 HV   41.1 HRC   1299 N/mm2
 384 HB   404 HV   41.2 HRC   1302 N/mm2
 385 HB   405 HV   41.3 HRC   1305 N/mm2
 386 HB   406 HV   41.4 HRC   1308 N/mm2
 387 HB   407 HV   41.5 HRC   1311 N/mm2
 388 HB   408 HV   41.6 HRC   1314 N/mm2
 389 HB   409 HV   41.7 HRC   1317 N/mm2
 390 HB   410 HV   41.8 HRC   1320 N/mm2
 391 HB   411 HV   41.9 HRC   1324 N/mm2
 392 HB   412 HV   42.0 HRC   1328 N/mm2
 393 HB   413 HV   42.1 HRC   1332 N/mm2
 394 HB   414 HV   42.2 HRC   1335 N/mm2
 395 HB   415 HV   42.3 HRC   1338 N/mm2
 396 HB   416 HV   42.4 HRC   1342 N/mm2
 397 HB   417 HV   42.5 HRC   1345 N/mm2
 398 HB   418 HV   42.6 HRC   1347 N/mm2
 399 HB   420 HV   42.7 HRC   1350 N/mm2
 400 HB   421 HV   42.8 HRC   1353 N/mm2
 401 HB   422 HV   42.9 HRC   1357 N/mm2
 402 HB   423 HV   43.0 HRC   1360 N/mm2
 403 HB   424 HV   43.1 HRC   1364 N/mm2
 404 HB   425 HV   43.2 HRC   1367 N/mm2
 405 HB   426 HV   43.3 HRC   1371 N/mm2
 406 HB   427 HV   43.4 HRC   1373 N/mm2
 407 HB   428 HV   43.5 HRC   1377 N/mm2
 408 HB   429 HV   43.5 HRC   1381 N/mm2
 409 HB   430 HV   43.6 HRC   1385 N/mm2
 410 HB   431 HV   43.7 HRC   1389 N/mm2
 411 HB   432 HV   43.8 HRC   1393 N/mm2
 412 HB   433 HV   43.9 HRC   1397 N/mm2
 413 HB   434 HV   44.0 HRC   1400 N/mm2
 414 HB   435 HV   44.1 HRC   1404 N/mm2
 415 HB   436 HV   44.2 HRC   1407 N/mm2
 416 HB   437 HV   44.3 HRC   1411 N/mm2
 417 HB   438 HV   44.4 HRC   1415 N/mm2
 418 HB   440 HV   44.5 HRC   1420 N/mm2
 419 HB   441 HV   44.6 HRC   1424 N/mm2
 420 HB   442 HV   44.7 HRC   1427 N/mm2
 421 HB   443 HV   44.8 HRC   1431 N/mm2
 422 HB   444 HV   44.9 HRC   1434 N/mm2
 423 HB   445 HV   45.0 HRC   1437 N/mm2
 424 HB   446 HV   45.1 HRC   1441 N/mm2
 425 HB   447 HV   45.1 HRC   1445 N/mm2
 426 HB   448 HV   45.2 HRC   1448 N/mm2
 427 HB   449 HV   45.2 HRC   1452 N/mm2
 428 HB   450 HV   45.3 HRC   1455 N/mm2
 429 HB   451 HV   45.3 HRC   1458 N/mm2
 430 HB   452 HV   45.4 HRC   1461 N/mm2
 431 HB   453 HV   45.5 HRC   1464 N/mm2
 432 HB   454 HV   45.6 HRC   1468 N/mm2
 433 HB   455 HV   45.7 HRC   1471 N/mm2
 434 HB   456 HV   45.8 HRC   1474 N/mm2
 435 HB   457 HV   45.9 HRC   1478 N/mm2
 436 HB   458 HV   46.0 HRC   1482 N/mm2
 437 HB   460 HV   46.1 HRC   1485 N/mm2
 438 HB   461 HV   46.2 HRC   1488 N/mm2
 439 HB   462 HV   46.3 HRC   1491 N/mm2
 440 HB   463 HV   46.4 HRC   1494 N/mm2
 441 HB   464 HV   46.5 HRC   1498 N/mm2
 442 HB   465 HV   46.6 HRC   1502 N/mm2
 443 HB   466 HV   46.6 HRC   1506 N/mm2
 444 HB   467 HV   46.7 HRC   1509 N/mm2
 445 HB   468 HV   46.7 HRC   1512 N/mm2
 446 HB   469 HV   46.8 HRC   1516 N/mm2
 447 HB   470 HV   46.9 HRC   1520 N/mm2
 448 HB   471 HV   47.0 HRC   1524 N/mm2
 449 HB   472 HV   47.1 HRC   1528 N/mm2
 450 HB   473 HV   47.1 HRC   1532 N/mm2
 451 HB   474 HV   47.2 HRC   1534 N/mm2
 452 HB   475 HV   47.3 HRC   1538 N/mm2
 453 HB   476 HV   47.4 HRC   1542 N/mm2
 454 HB   477 HV   47.5 HRC   1546 N/mm2
 455 HB   478 HV   47.6 HRC   1550 N/mm2
 456 HB   480 HV   47.7 HRC   1555 N/mm2
 457 HB   481 HV   47.7 HRC   1559 N/mm2
 458 HB   482 HV   47.8 HRC   1563 N/mm2
 459 HB   483 HV   47.9 HRC   1567 N/mm2
 460 HB   484 HV   47.9 HRC   1571 N/mm2
 461 HB   485 HV   48.0 HRC   1575 N/mm2
 462 HB   486 HV   48.1 HRC   1579 N/mm2
 463 HB   487 HV   48.2 HRC   1583 N/mm2
 464 HB   488 HV   48.3 HRC   1587 N/mm2
 465 HB   489 HV   48.3 HRC   1591 N/mm2
 466 HB   490 HV   48.4 HRC   1595 N/mm2
 467 HB   491 HV   48.4 HRC   1599 N/mm2
 468 HB   492 HV   48.5 HRC   1603 N/mm2
 469 HB   493 HV   48.5 HRC   1607 N/mm2
 470 HB   494 HV   48.6 HRC   1611 N/mm2
 471 HB   495 HV   48.7 HRC   1614 N/mm2
 472 HB   496 HV   48.8 HRC   1618 N/mm2
 473 HB   497 HV   48.9 HRC   1622 N/mm2
 474 HB   498 HV   49.0 HRC   1626 N/mm2
 475 HB   500 HV   49.1 HRC   1630 N/mm2
 476 HB   501 HV   49.2 HRC   1633 N/mm2
 477 HB   502 HV   49.2 HRC   1637 N/mm2
 478 HB   503 HV   49.3 HRC   1640 N/mm2
 479 HB   504 HV   49.4 HRC   1643 N/mm2
 480 HB   505 HV   49.5 HRC   1644 N/mm2
 481 HB   506 HV   49.5 HRC   1647 N/mm2
 482 HB   507 HV   49.6 HRC   1651 N/mm2
 483 HB   508 HV   49.7 HRC   1655 N/mm2
 484 HB   509 HV   49.7 HRC   1660 N/mm2
 485 HB   510 HV   49.8 HRC   1665 N/mm2
 486 HB   511 HV   49.9 HRC   1669 N/mm2
 487 HB   512 HV   49.9 HRC   1673 N/mm2
 488 HB   513 HV   50.0 HRC   1677 N/mm2
 489 HB   514 HV   50.1 HRC   1681 N/mm2
 490 HB   515 HV   50.2 HRC   1685 N/mm2
 491 HB   516 HV   50.3 HRC   1689 N/mm2
 492 HB   517 HV   50.3 HRC   1693 N/mm2
 493 HB   518 HV   50.4 HRC   1697 N/mm2
 494 HB   520 HV   50.5 HRC   1700 N/mm2
 495 HB   521 HV   50.5 HRC   1704 N/mm2
 496 HB   522 HV   50.6 HRC   1708 N/mm2
 497 HB   523 HV   50.6 HRC   1712 N/mm2
 498 HB   524 HV   50.7 HRC   1716 N/mm2
 499 HB   525 HV   50.7 HRC   1720 N/mm2
 500 HB   526 HV   50.8 HRC   1724 N/mm2
 501 HB   527 HV   50.8 HRC   1728 N/mm2
 502 HB   528 HV   50.9 HRC   1732 N/mm2
 503 HB   529 HV   51.0 HRC   1736 N/mm2
 504 HB   530 HV   51.1 HRC   1740 N/mm2
 505 HB   531 HV   51.1 HRC   1744 N/mm2
 506 HB   532 HV   51.2 HRC   1748 N/mm2
 507 HB   533 HV   51.2 HRC   1752 N/mm2
 508 HB   534 HV   51.3 HRC   1756 N/mm2
 509 HB   535 HV   51.4 HRC   1760 N/mm2
 510 HB   536 HV   51.5 HRC   1764 N/mm2
 511 HB   537 HV   51.5 HRC   1768 N/mm2
 512 HB   538 HV   51.6 HRC   1772 N/mm2
 513 HB   540 HV   51.7 HRC   1775 N/mm2
 514 HB   541 HV   51.7 HRC   1779 N/mm2
 515 HB   542 HV   51.8 HRC   1782 N/mm2
 516 HB   543 HV   51.8 HRC   1786 N/mm2
 517 HB   544 HV   51.9 HRC   1789 N/mm2
 518 HB   545 HV   51.9 HRC   1793 N/mm2
 519 HB   546 HV   52.0 HRC   1797 N/mm2
 520 HB   547 HV   52.0 HRC   1801 N/mm2
 521 HB   548 HV   52.1 HRC   1804 N/mm2
 522 HB   549 HV   52.2 HRC   1807 N/mm2
 523 HB   550 HV   52.3 HRC   1810 N/mm2
 524 HB   551 HV   52.3 HRC   1814 N/mm2
 525 HB   552 HV   52.4 HRC   1818 N/mm2
 526 HB   553 HV   52.4 HRC   1822 N/mm2
 527 HB   554 HV   52.5 HRC   1826 N/mm2
 528 HB   555 HV   52.6 HRC   1830 N/mm2
 529 HB   556 HV   52.7 HRC   1834 N/mm2
 530 HB   557 HV   52.8 HRC   1838 N/mm2
 531 HB   558 HV   52.9 HRC   1842 N/mm2
 532 HB   560 HV   53.0 HRC   1845 N/mm2
 533 HB   561 HV   53.0 HRC   1848 N/mm2
 534 HB   562 HV   53.1 HRC   1852 N/mm2
 535 HB   563 HV   53.1 HRC   1855 N/mm2
 536 HB   564 HV   53.2 HRC   1859 N/mm2
 537 HB   565 HV   53.2 HRC   1863 N/mm2
 538 HB   566 HV   53.3 HRC   1867 N/mm2
 539 HB   567 HV   53.3 HRC   1870 N/mm2
 540 HB   568 HV   53.4 HRC   1873 N/mm2
 541 HB   569 HV   53.5 HRC   1876 N/mm2
 542 HB   570 HV   53.6 HRC   1880 N/mm2
 543 HB   571 HV   53.6 HRC   1884 N/mm2
 544 HB   571 HV   53.7 HRC   1889 N/mm2
 545 HB   573 HV   53.7 HRC   1893 N/mm2
 546 HB   574 HV   53.8 HRC   1898 N/mm2
 547 HB   575 HV   53.8 HRC   1902 N/mm2
 548 HB   576 HV   53.9 HRC   1907 N/mm2
 549 HB   577 HV   53.9 HRC   1912 N/mm2
 550 HB   578 HV   54.0 HRC   1916 N/mm2
 551 HB   580 HV   54.1 HRC   1920 N/mm2
 552 HB   581 HV   54.1 HRC   1923 N/mm2
 553 HB   582 HV   54.2 HRC   1927 N/mm2
 554 HB   583 HV   54.2 HRC   1930 N/mm2
 555 HB   584 HV   54.3 HRC   1934 N/mm2
 556 HB   585 HV   54.3 HRC   1937 N/mm2
 557 HB   586 HV   54.4 HRC   1941 N/mm2
 558 HB   587 HV   54.4 HRC   1945 N/mm2
 559 HB   588 HV   54.5 HRC   1948 N/mm2
 560 HB   589 HV   54.6 HRC   1952 N/mm2
 561 HB   590 HV   54.7 HRC   1955 N/mm2
 562 HB   591 HV   54.7 HRC   1959 N/mm2
 563 HB   592 HV   54.8 HRC   1964 N/mm2
 564 HB   593 HV   54.8 HRC   1969 N/mm2
 565 HB   594 HV   54.9 HRC   1973 N/mm2
 566 HB   595 HV   54.9 HRC   1978 N/mm2
 567 HB   596 HV   55.0 HRC   1982 N/mm2
 568 HB   597 HV   55.1 HRC   1987 N/mm2
 569 HB   598 HV   55.1 HRC   1991 N/mm2
 570 HB   600 HV   55.2 HRC   1995 N/mm2
 571 HB   601 HV   55.2 HRC   1999 N/mm2
 572 HB   602 HV   55.3 HRC   2002 N/mm2
 573 HB   603 HV   55.3 HRC   2006 N/mm2
 574 HB   604 HV   55.4 HRC   2009 N/mm2
 575 HB   605 HV   55.4 HRC   2013 N/mm2
 576 HB   606 HV   55.5 HRC   2016 N/mm2
 577 HB   607 HV   55.5 HRC   2020 N/mm2
 578 HB   608 HV   55.6 HRC   2023 N/mm2
 579 HB   609 HV   55.6 HRC   2027 N/mm2
 580 HB   610 HV   55.7 HRC   2030 N/mm2
 581 HB   611 HV   55.7 HRC   2034 N/mm2
 582 HB   612 HV   55.8 HRC   2039 N/mm2
 583 HB   613 HV   55.8 HRC   2043 N/mm2
 584 HB   614 HV   55.9 HRC   2048 N/mm2
 585 HB   615 HV   55.9 HRC   2052 N/mm2
 586 HB   616 HV   56.0 HRC   2057 N/mm2
 587 HB   617 HV   56.1 HRC   2061 N/mm2
 588 HB   618 HV   56.2 HRC   2065 N/mm2
 589 HB   620 HV   56.3 HRC   2070 N/mm2
 590 HB   621 HV   56.3 HRC   2073 N/mm2
 591 HB   622 HV   56.4 HRC   2077 N/mm2
 592 HB   623 HV   56.4 HRC   2080 N/mm2
 593 HB   624 HV   56.5 HRC   2084 N/mm2
 594 HB   625 HV   56.5 HRC   2087 N/mm2
 595 HB   626 HV   56.6 HRC   2091 N/mm2
 596 HB   627 HV   56.6 HRC   2093 N/mm2
 597 HB   628 HV   56.7 HRC   2097 N/mm2
 598 HB   629 HV   56.7 HRC   2101 N/mm2
 599 HB   630 HV   56.8 HRC   2105 N/mm2
 600 HB   631 HV   56.8 HRC   2109 N/mm2
 601 HB   632 HV   56.9 HRC   2114 N/mm2
 602 HB   633 HV   56.9 HRC   2118 N/mm2
 603 HB   634 HV   57.0 HRC   2123 N/mm2
 604 HB   635 HV   57.0 HRC   2127 N/mm2
 605 HB   636 HV   57.1 HRC   2132 N/mm2
 606 HB   637 HV   57.2 HRC   2136 N/mm2
 607 HB   638 HV   57.2 HRC   2141 N/mm2
 608 HB   640 HV   57.3 HRC   2145 N/mm2
 609 HB   641 HV   57.3 HRC   2148 N/mm2
 610 HB   642 HV   57.4 HRC   2152 N/mm2
 611 HB   643 HV   57.4 HRC   2155 N/mm2
 612 HB   644 HV   57.5 HRC   2159 N/mm2
 613 HB   645 HV   57.5 HRC   2162 N/mm2
 614 HB   646 HV   57.6 HRC   2166 N/mm2
 615 HB   647 HV   57.6 HRC   2169 N/mm2
 616 HB   648 HV   57.7 HRC   2173 N/mm2
 617 HB   649 HV   57.7 HRC   2177 N/mm2
 618 HB   650 HV   57.8 HRC   2180 N/mm2
 – HB   651 HV   57.8 HRC   – N/mm2
 – HB   652 HV   57.8 HRC   – N/mm2
 – HB   653 HV   57.9 HRC   – N/mm2
 – HB   654 HV   57.9 HRC   – N/mm2
 – HB   655 HV   58.0 HRC   – N/mm2
 – HB   656 HV   58.0 HRC   – N/mm2
 – HB   657 HV   58.1 HRC   – N/mm2
 – HB   658 HV   58.1 HRC   – N/mm2
 – HB   660 HV   58.3 HRC   – N/mm2
 – HB   661 HV   58.3 HRC   – N/mm2
 – HB   662 HV   58.4 HRC   – N/mm2
 – HB   663 HV   58.4 HRC   – N/mm2
 – HB   664 HV   58.5 HRC   – N/mm2
 – HB   665 HV   58.5 HRC   – N/mm2
 – HB   666 HV   58.6 HRC   – N/mm2
 – HB   667 HV   58.6 HRC   – N/mm2
 – HB   668 HV   58.7 HRC   – N/mm2
 – HB   669 HV   58.7 HRC   – N/mm2
 – HB   670 HV   58.8 HRC   – N/mm2
 – HB   671 HV   58.8 HRC   – N/mm2
 – HB   672 HV   58.9 HRC   – N/mm2
 – HB   673 HV   58.9 HRC   – N/mm2
 – HB   674 HV   59.0 HRC   – N/mm2
 – HB   675 HV   59.0 HRC   – N/mm2
 – HB   676 HV   59.0 HRC   – N/mm2
 – HB   677 HV   59.1 HRC   – N/mm2
 – HB   678 HV   59.1 HRC   – N/mm2
 – HB   679 HV   59.1 HRC   – N/mm2
 – HB   680 HV   59.2 HRC   – N/mm2
 – HB   681 HV   59.2 HRC   – N/mm2
 – HB   682 HV   59.3 HRC   – N/mm2
 – HB   683 HV   59.3 HRC   – N/mm2
 – HB   684 HV   59.4 HRC   – N/mm2
 – HB   685 HV   59.4 HRC   – N/mm2
 – HB   686 HV   59.5 HRC   – N/mm2
 – HB   687 HV   59.5 HRC   – N/mm2
 – HB   688 HV   59.6 HRC   – N/mm2
 – HB   689 HV   59.6 HRC   – N/mm2
 – HB   690 HV   59.7 HRC   – N/mm2
 – HB   691 HV   59.7 HRC   – N/mm2
 – HB   692 HV   59.8 HRC   – N/mm2
 – HB   693 HV   59.8 HRC   – N/mm2
 – HB   694 HV   59.9 HRC   – N/mm2
 – HB   695 HV   59.9 HRC   – N/mm2
 – HB   696 HV   59.9 HRC   – N/mm2
 – HB   697 HV   60.0 HRC   – N/mm2
 – HB   698 HV   60.0 HRC   – N/mm2
 – HB   699 HV   60.0 HRC   – N/mm2
 – HB   700 HV   60.1 HRC   – N/mm2
 – HB   701 HV   60.1 HRC   – N/mm2
 – HB   702 HV   60.2 HRC   – N/mm2
 – HB   703 HV   60.2 HRC   – N/mm2
 – HB   704 HV   60.2 HRC   – N/mm2
 – HB   705 HV   60.3 HRC   – N/mm2
 – HB   706 HV   60.3 HRC   – N/mm2
 – HB   707 HV   60.4 HRC   – N/mm2
 – HB   708 HV   60.4 HRC   – N/mm2
 – HB   709 HV   60.5 HRC   – N/mm2
 – HB   710 HV   60.5 HRC   – N/mm2
 – HB   711 HV   60.6 HRC   – N/mm2
 – HB   712 HV   60.6 HRC   – N/mm2
 – HB   713 HV   60.7 HRC   – N/mm2
 – HB   714 HV   60.7 HRC   – N/mm2
 – HB   715 HV   60.8 HRC   – N/mm2
 – HB   716 HV   60.8 HRC   – N/mm2
 – HB   717 HV   60.8 HRC   – N/mm2
 – HB   718 HV   60.9 HRC   – N/mm2
 – HB   719 HV   60.9 HRC   – N/mm2
 – HB   720 HV   61.0 HRC   – N/mm2
 – HB   721 HV   61.0 HRC   – N/mm2
 – HB   722 HV   61.1 HRC   – N/mm2
 – HB   723 HV   61.1 HRC   – N/mm2
 – HB   724 HV   61.2 HRC   – N/mm2
 – HB   725 HV   61.2 HRC   – N/mm2
 – HB   726 HV   61.3 HRC   – N/mm2
 – HB   727 HV   61.3 HRC   – N/mm2
 – HB   728 HV   61.4 HRC   – N/mm2
 – HB   729 HV   61.4 HRC   – N/mm2
 – HB   730 HV   61.5 HRC   – N/mm2
 – HB   731 HV   61.5 HRC   – N/mm2
 – HB   732 HV   61.6 HRC   – N/mm2
 – HB   733 HV   61.6 HRC   – N/mm2
 – HB   734 HV   61.6 HRC   – N/mm2
 – HB   735 HV   61.6 HRC   – N/mm2
 – HB   736 HV   61.7 HRC   – N/mm2
 – HB   737 HV   61.7 HRC   – N/mm2
 – HB   738 HV   61.7 HRC   – N/mm2
 – HB   739 HV   61.7 HRC   – N/mm2
 – HB   740 HV   61.8 HRC   – N/mm2
 – HB   741 HV   61.8 HRC   – N/mm2
 – HB   742 HV   61.8 HRC   – N/mm2
 – HB   743 HV   61.8 HRC   – N/mm2
 – HB   744 HV   61.9 HRC   – N/mm2
 – HB   745 HV   61.9 HRC   – N/mm2
 – HB   746 HV   61.9 HRC   – N/mm2
 – HB   747 HV   62.0 HRC   – N/mm2
 – HB   748 HV   62.0 HRC   – N/mm2
 – HB   749 HV   62.0 HRC   – N/mm2
 – HB   750 HV   62.1 HRC   – N/mm2
 – HB   751 HV   62.1 HRC   – N/mm2
 – HB   752 HV   62.1 HRC   – N/mm2
 – HB   753 HV   62.2 HRC   – N/mm2
 – HB   754 HV   62.2 HRC   – N/mm2
 – HB   755 HV   62.2 HRC   – N/mm2
 – HB   756 HV   62.3 HRC   – N/mm2
 – HB   757 HV   62.3 HRC   – N/mm2
 – HB   758 HV   62.4 HRC   – N/mm2
 – HB   759 HV   62.4 HRC   – N/mm2
 – HB   760 HV   62.5 HRC   – N/mm2
 – HB   761 HV   62.5 HRC   – N/mm2
 – HB   762 HV   62.5 HRC   – N/mm2
 – HB   763 HV   62.6 HRC   – N/mm2
 – HB   764 HV   62.6 HRC   – N/mm2
 – HB   765 HV   62.6 HRC   – N/mm2
 – HB   766 HV   62.7 HRC   – N/mm2
 – HB   767 HV   62.7 HRC   – N/mm2
 – HB   768 HV   62.7 HRC   – N/mm2
 – HB   769 HV   62.8 HRC   – N/mm2
 – HB   770 HV   62.8 HRC   – N/mm2
 – HB   771 HV   62.9 HRC   – N/mm2
 – HB   772 HV   62.9 HRC   – N/mm2
 – HB   773 HV   63.0 HRC   – N/mm2
 – HB   774 HV   63.0 HRC   – N/mm2
 – HB   775 HV   63.1 HRC   – N/mm2
 – HB   776 HV   63.1 HRC   – N/mm2
 – HB   777 HV   63.1 HRC   – N/mm2
 – HB   778 HV   63.2 HRC   – N/mm2
 – HB   779 HV   63.2 HRC   – N/mm2
 – HB   780 HV   63.3 HRC   – N/mm2
 – HB   781 HV   63.3 HRC   – N/mm2
 – HB   782 HV   63.3 HRC   – N/mm2
 – HB   783 HV   63.4 HRC   – N/mm2
 – HB   784 HV   63.4 HRC   – N/mm2
 – HB   785 HV   63.4 HRC   – N/mm2
 – HB   786 HV   63.5 HRC   – N/mm2
 – HB   787 HV   63.5 HRC   – N/mm2
 – HB   788 HV   63.5 HRC   – N/mm2
 – HB   789 HV   63.6 HRC   – N/mm2
 – HB   790 HV   63.6 HRC   – N/mm2
 – HB   791 HV   63.6 HRC   – N/mm2
 – HB   792 HV   63.7 HRC   – N/mm2
 – HB   793 HV   63.7 HRC   – N/mm2
 – HB   794 HV   63.7 HRC   – N/mm2
 – HB   795 HV   63.8 HRC   – N/mm2
 – HB   796 HV   63.8 HRC   – N/mm2
 – HB   797 HV   63.8 HRC   – N/mm2
 – HB   798 HV   63.9 HRC   – N/mm2
 – HB   799 HV   63.9 HRC   – N/mm2
 – HB   800 HV   64.0 HRC   – N/mm2
 – HB   801 HV   64.1 HRC   – N/mm2
 – HB   802 HV   64.1 HRC   – N/mm2
 – HB   803 HV   64.1 HRC   – N/mm2
 – HB   804 HV   64.2 HRC   – N/mm2
 – HB   805 HV   64.2 HRC   – N/mm2
 – HB   806 HV   64.2 HRC   – N/mm2
 – HB   807 HV   64.3 HRC   – N/mm2
 – HB   808 HV   64.3 HRC   – N/mm2
 – HB   809 HV   64.3 HRC   – N/mm2
 – HB   810 HV   64.4 HRC   – N/mm2
 – HB   811 HV   64.4 HRC   – N/mm2
 – HB   812 HV   64.4 HRC   – N/mm2
 – HB   813 HV   64.4 HRC   – N/mm2
 – HB   814 HV   64.5 HRC   – N/mm2
 – HB   815 HV   64.5 HRC   – N/mm2
 – HB   816 HV   64.5 HRC   – N/mm2
 – HB   817 HV   64.6 HRC   – N/mm2
 – HB   818 HV   64.6 HRC   – N/mm2
 – HB   819 HV   64.6 HRC   – N/mm2
 – HB   820 HV   64.7 HRC   – N/mm2
 – HB   821 HV   64.7 HRC   – N/mm2
 – HB   822 HV   64.7 HRC   – N/mm2
 – HB   823 HV   64.8 HRC   – N/mm2
 – HB   824 HV   64.8 HRC   – N/mm2
 – HB   825 HV   64.8 HRC   – N/mm2
 – HB   826 HV   64.8 HRC   – N/mm2
 – HB   827 HV   64.9 HRC   – N/mm2
 – HB   828 HV   64.9 HRC   – N/mm2
 – HB   829 HV   64.9 HRC   – N/mm2
 – HB   830 HV   65.0 HRC   – N/mm2
 – HB   831 HV   65.0 HRC   – N/mm2
 – HB   832 HV   65.0 HRC   – N/mm2
 – HB   833 HV   65.0 HRC   – N/mm2
 – HB   834 HV   65.1 HRC   – N/mm2
 – HB   835 HV   65.1 HRC   – N/mm2
 – HB   836 HV   65.1 HRC   – N/mm2
 – HB   837 HV   65.2 HRC   – N/mm2
 – HB   838 HV   65.2 HRC   – N/mm2
 – HB   839 HV   65.2 HRC   – N/mm2
 – HB   840 HV   65.3 HRC   – N/mm2
 – HB   841 HV   65.3 HRC   – N/mm2
 – HB   842 HV   65.3 HRC   – N/mm2
 – HB   843 HV   65.4 HRC   – N/mm2
 – HB   844 HV   65.4 HRC   – N/mm2
 – HB   845 HV   65.4 HRC   – N/mm2
 – HB   846 HV   65.5 HRC   – N/mm2
 – HB   847 HV   65.5 HRC   – N/mm2
 – HB   848 HV   65.5 HRC   – N/mm2
 – HB   849 HV   65.5 HRC   – N/mm2
 – HB   850 HV   65.6 HRC   – N/mm2
 – HB   851 HV   65.6 HRC   – N/mm2
 – HB   852 HV   65.6 HRC   – N/mm2
 – HB   853 HV   65.7 HRC   – N/mm2
 – HB   854 HV   65.7 HRC   – N/mm2
 – HB   855 HV   65.7 HRC   – N/mm2
 – HB   856 HV   65.8 HRC   – N/mm2
 – HB   857 HV   65.8 HRC   – N/mm2
 – HB   858 HV   65.8 HRC   – N/mm2
 – HB   859 HV   65.9 HRC   – N/mm2
 – HB   860 HV   65.9 HRC   – N/mm2
 – HB   861 HV   65.9 HRC   – N/mm2
 – HB   862 HV   65.9 HRC   – N/mm2
 – HB   863 HV   66.0 HRC   – N/mm2
 – HB   864 HV   66.0 HRC   – N/mm2
 – HB   865 HV   66.0 HRC   – N/mm2
 – HB   866 HV   66.0 HRC   – N/mm2
 – HB   867 HV   66.1 HRC   – N/mm2
 – HB   868 HV   66.1 HRC   – N/mm2
 – HB   869 HV   66.1 HRC   – N/mm2
 – HB   870 HV   66.1 HRC   – N/mm2
 – HB   871 HV   66.2 HRC   – N/mm2
 – HB   872 HV   66.2 HRC   – N/mm2
 – HB   873 HV   66.2 HRC   – N/mm2
 – HB   874 HV   66.2 HRC   – N/mm2
 – HB   875 HV   66.3 HRC   – N/mm2
 – HB   876 HV   66.3 HRC   – N/mm2
 – HB   877 HV   66.3 HRC   – N/mm2
 – HB   878 HV   66.3 HRC   – N/mm2
 – HB   879 HV   66.4 HRC   – N/mm2
 – HB   880 HV   66.4 HRC   – N/mm2
 – HB   881 HV   66.4 HRC   – N/mm2
 – HB   882 HV   66.4 HRC   – N/mm2
 – HB   883 HV   66.5 HRC   – N/mm2
 – HB   884 HV   66.5 HRC   – N/mm2
 – HB   885 HV   66.5 HRC   – N/mm2
 – HB   886 HV   66.5 HRC   – N/mm2
 – HB   887 HV   66.5 HRC   – N/mm2
 – HB   888 HV   66.6 HRC   – N/mm2
 – HB   889 HV   66.6 HRC   – N/mm2
 – HB   890 HV   66.6 HRC   – N/mm2
 – HB   891 HV   66.7 HRC   – N/mm2
 – HB   892 HV   66.7 HRC   – N/mm2
 – HB   893 HV   66.7 HRC   – N/mm2
 – HB   894 HV   66.7 HRC   – N/mm2
 – HB   895 HV   66.8 HRC   – N/mm2
 – HB   896 HV   66.8 HRC   – N/mm2
 – HB   897 HV   66.8 HRC   – N/mm2
 – HB   898 HV   66.9 HRC   – N/mm2
 – HB   899 HV   66.9 HRC   – N/mm2
 – HB   900 HV   67.0 HRC   – N/mm2
 – HB   901 HV   67.0 HRC   – N/mm2
 – HB   902 HV   67.0 HRC   – N/mm2
 – HB   903 HV   67.0 HRC   – N/mm2
 – HB   904 HV   67.0 HRC   – N/mm2
 – HB   905 HV   67.1 HRC   – N/mm2
 – HB   906 HV   67.1 HRC   – N/mm2
 – HB   907 HV   67.1 HRC   – N/mm2
 – HB   908 HV   67.1 HRC   – N/mm2
 – HB   909 HV   67.2 HRC   – N/mm2
 – HB   910 HV   67.2 HRC   – N/mm2
 – HB   911 HV   67.2 HRC   – N/mm2
 – HB   912 HV   67.2 HRC   – N/mm2
 – HB   913 HV   67.2 HRC   – N/mm2
 – HB   914 HV   67.3 HRC   – N/mm2
 – HB   915 HV   67.3 HRC   – N/mm2
 – HB   916 HV   67.3 HRC   – N/mm2
 – HB   917 HV   67.4 HRC   – N/mm2
 – HB   918 HV   67.4 HRC   – N/mm2
 – HB   919 HV   67.4 HRC   – N/mm2
 – HB   920 HV   67.5 HRC   – N/mm2
 – HB   921 HV   67.5 HRC   – N/mm2
 – HB   921 HV   67.5 HRC   – N/mm2
 – HB   923 HV   67.5 HRC   – N/mm2
 – HB   924 HV   67.6 HRC   – N/mm2
 – HB   925 HV   67.6 HRC   – N/mm2
 – HB   926 HV   67.6 HRC   – N/mm2
 – HB   927 HV   67.6 HRC   – N/mm2
 – HB   928 HV   67.7 HRC   – N/mm2
 – HB   929 HV   67.7 HRC   – N/mm2
 – HB   930 HV   67.7 HRC   – N/mm2
 – HB   931 HV   67.7 HRC   – N/mm2
 – HB   932 HV   67.8 HRC   – N/mm2
 – HB   933 HV   67.8 HRC   – N/mm2
 – HB   934 HV   67.8 HRC   – N/mm2
 – HB   935 HV   67.8 HRC   – N/mm2
 – HB   936 HV   67.9 HRC   – N/mm2
 – HB   937 HV   67.9 HRC   – N/mm2
 – HB   938 HV   67.9 HRC   – N/mm2
 – HB   939 HV   67.9 HRC   – N/mm2
 – HB   940 HV   68.0 HRC   – N/mm2

About Us

Founded in 1998, FuShun covers an area of 3000 square meters, annual sales volume of 20000 tons. We are engaged in the manufacture and export of Tool Steel, Nickel Alloy, Stainless Steel and other special steel products…,View more content About Me.

Get A Free Quote!

Fushun TEL: +86-731-89903933

Fushun FAX: +86-731-89853933

General Manager: Ms. Florence Tang

Whatsapp/Phone/WeChat:+86-13319591838

Find your steel grade and get a quote today.

NOW Send Your Inquiry To : info@fushunspecialsteel.com

Whatsapp:+86-18692275455

x