1.4935, X20CRMOWV12-1, AISI 422, CREEP RESISTING STEEL

1.4935, X20CRMOWV12-1, AISI 422 – CREEP RESISTING STEEL

Material 1.4935 High-temperature resisting steel and alloy. The material 1.4935 is a highly heat-resistant martensitic steel. This steel can be used up to a maximum temperature of about 650 °C / 1202 °F. Typical application for the turbine is 1.4935.

 

Standards

HDIN / EN US-Standard
X20CrMoWV12-1 AISI 422 UNS S42200

 

Chemical Composition

Standard C: Si: Mn: P: S: Cr: Mo: Ni: V: W: Cu:
EN 1.4935, X20CrMoWV12-1
0.17-0.24 0.1-0.5 0.3-0.8 <0.025 <0.015 11.0-12.5 0.8-1.2 0.3-0.8 0.25-0.35 0.4-0.6
JIS SUH616
0.20-0.25 <0.5 0.5-1.0 <0.04 <0.03 11.0-13.0 0.75-1.25 0.5-1.0 0.2-0.3 0.75-1.25 <0.3
ASTM AISI 422 / AISI 616 – S42200
0.20-0.25 <0.75 <1.0 <0.04 <0.03 11.0-12.5 0.75-1.25 0.5-1.0 0.15-0.30 0.75-1.25 <0.5

 

 

APPLICATIONS

Jet engine components

High temperature fasteners, springs

Non-magnetic cryogenic equipment

 

1.4935, X20CRMOWV12-1, AISI 422 – CREEP RESISTING STEEL, DATA ACCORDING TO EN 10088-3:2014 AND EN 10302

 

1.4935, X20CrMoWV12-1 – description

Creep resistant steel used for thermal engine components in power plants, mainly turbine blades, but fasteners as well. Hardenable. Max temperature for continous operating is 580 °C.

Chrome-nickel steel with an austenitic structure with carbides. Alloying additions of molybdenum, vanadium and tungsten increase the melting temperature, thus having a positive effect on creep resistance.

The steel is hard to weld. It is assigned to welding group 7.2 according to ISO/TR 20172.

 

Physical and mechanical properties

1.4935 – physical properties and indicative mechanical properties:

Density: 7.7 g/cm3

Linear expansion coefficient: 10.5-12.5 *10-6m/(m*K)

Thermal conductivity: 24 W/(m*K)

Specific heat capacity: 460 J/(kg*K)

Young’s modulus: 216 GPa

Electrical resistivity: 0.6 µΩ*m

Tensile strength Rm: > 600 MPa

Creep limit for max elongation 0.2% Rp0.2: > 800 MPa

Creep-rupture strength Ru: > 275 MPa; 500 °C; 100000 h

Creep limit for max elongation 0.2% Rp0.2 – high temperature test:

Testing temperature: 400 °C – > 420 MPa

Testing temperature: 500 °C – > 335 MPa

 

Mechanical properties of +QT700 class forgings:

Ambient temperature:

Re: > 500 MPa

Rm: 700-850 MPa

A: 15 %

 

Yield strength Re in high temperature:

Testing temperature: 50 °C – > 465 MPa

Testing temperature: 100 °C – > 460 MPa

Testing temperature: 150 °C – > 445 MPa

Testing temperature: 200 °C – > 430 MPa

Testing temperature: 250 °C – > 415 MPa

Testing temperature: 300 °C – > 390 MPa

Testing temperature: 350 °C – > 380 MPa

Testing temperature: 400 °C – > 360 MPa

Testing temperature: 450 °C – > 330 MPa

Testing temperature: 500 °C – > 290 MPa

Testing temperature: 550 °C – > 250 MPa

 

Mechanical properties of +QT800 class forgings:

Ambient temperature:

Re: > 600 MPa

Rm: 800-950 MPa

A: 14 %

 

Yield strength Re in high temperature:

Testing temperature: 50 °C – > 585 MPa

Testing temperature: 100 °C – > 560 MPa

Testing temperature: 150 °C – > 545 MPa

Testing temperature: 200 °C – > 530 MPa

Testing temperature: 250 °C – > 505 MPa

Testing temperature: 300 °C – > 480 MPa

Testing temperature: 350 °C – > 450 MPa

Testing temperature: 400 °C – > 420 MPa

Testing temperature: 450 °C – > 380 MPa

Testing temperature: 500 °C – > 335 MPa

Testing temperature: 550 °C – > 280 MPa

 

Heat treatment and working

Recommended working and heat treatment parameters for 1.4935 alloy:

Quenching: 1020-1070 °C

Tempering: 680-780 °C

 

Replacements, equivalents and other designations:

1.4935, X22CRMOWV12-1, SUH616, 20VNIWMOCR120, AISI 422, AISI 616, S42200, EW 4935, T502, 56B.I.; DE 4935, HWMOV3, GRADE 616

 

Machining Status

raw
Rough Turning
Finished
Processed according to technical drawing

 

About Us

Founded in 1998, FuShun covers an area of 3000 square meters, annual sales volume of 20000 tons. We are engaged in the manufacture and export of Tool Steel, Nickel Alloy, Stainless Steel and other special steel products…,View more content About Me.

Get A Free Quote!

Fushun TEL: +86-731-89903933

Fushun FAX: +86-731-89853933

General Manager: Ms. Florence Tang

Whatsapp/Phone/WeChat:+86-13319591838

Find your steel grade and get a quote today.

NOW Send Your Inquiry To : info@fushunspecialsteel.com

Whatsapp:+86-18692275455

x